HOME Technical Know-How Applications of Precision ceramic materials 주요내마모재
특성표 |
 |
 |
efficiency per unit |
 |
비교
단위 : $
Material |
Description |
COST
(□/Litre) |
Wea
Index |
Relative
Life |
Cost
(□/Unit Wear) |
Coromant |
Sintered Tungsten Carbide |
742.00 |
0.0275 |
36.36 |
20.407 |
Alumina Ceramic |
Fully Sintered Alumina |
4.00 |
0.0800 |
15.00 |
0.235 |
Duaplate |
Cr Plated Hard Facing |
24.00 |
0.2065 |
4.48 |
5.357 |
BF253 |
Hi Cr White Cast Iron |
5.19 |
0.2310 |
4.33 |
1.199 |
BF954 |
Ni Cr White Cast Iron |
4.8 |
0.4800 |
4.16 |
1.154 |
BF202 |
Cr Mo White Iron |
7.36 |
0.3310 |
3.02 |
2.437 |
Cast Basalt |
Volcanic Rock |
0.95 |
0.3780 |
2.64 |
0.360 |
Creusabro 32 |
Normalised Steel |
3.32 |
0.5290 |
1.90 |
1.747 |
EN8 |
Steel |
1.44 |
1.0000 |
1.00 |
1.440 |
EN58 |
312 Stainless Steel |
9.63 |
1.095 |
|
|
BS4360 |
Rolled Mild Steel |
AKT |
1.493 |
|
2.110 |
|
 |
physical characteristic & Abrasion Rate |
 |
Item |
Specific gravity |
hardness (HV) |
Compressive strength
(Kgf/㎠) |
Abrasion Rate |
Remarks |
Alumina |
3.7 |
1,110 |
24,000 |
1 |
|
용융현무암(BASALT) |
3.0 |
720 |
5,400 |
≒5배 |
|
Super Hard-steel for welding |
14.9 |
640 |
26,000 |
≒3∼5배 |
|
S45C |
7.86 |
137 |
12,000 |
≒18배 |
|
SUS304 |
8.02 |
295 |
- |
≒8∼10배 |
|
FC-20 |
7.75 |
171 |
6,500 |
≒12∼15배 |
|
Hi-Cr 강 |
7.53 |
355 |
- |
≒6∼8배 |
|
주)
1. Operation condition ? less than FLY ASH 4 18Kgf/㎠, Resistant material thickness 5t |
 |
Lifespan comparison for different uses |
 |
? item |
Standard Specification |
Operation condition |
Austenitic Manganese |
Super hard-steel |
Alumina |
BASALT |
cast iron |
FAN CASING |
2,232X420L |
670RPM |
5.5개월 |
20개월 |
36개월 |
7개월 |
- |
CHUTE |
1,000X700 |
석회석 2m낙하 |
- |
185,000톤 |
612,000톤 |
71,000톤 |
- |
ELBOW |
200X90° |
ASH 17m/Sec |
8개월 |
- |
84개월 |
17개월 |
3개월 |
INNER CONE |
2,685X1,585L |
137 |
- |
36개월 |
72개월 |
- |
- |